Re: Analysis of aluminum alloy sample Aurora TX
- From: "Martin H. Eastburn" <lionslair@xxxxxxxxxxxxxxxx>
- Date: Sun, 03 Feb 2008 21:51:49 -0600
I suppose you are saying ? moon men ?
Actually, there is a large Aluminum fab lines in operation - many engineers
have samples and junk. The other possibility is an early satellite breaking
up around there and over head... breakup trail. Also to the West is
White Sands. There they were sending rockets and missiles skyward and
blowing them up. Wonders ever cease - the winds would blow it Eastward.
I, being of high tech and of the Missile world for many years know that
target missiles fly high and when exploded do star bursts.
I suspect the sample was from a logical source but the finder and such were
not thinking of airplane or missile material. American or German in those days.
Martin
Martin H. Eastburn
@ home at Lions' Lair with our computer lionslair at consolidated dot net
TSRA, Endowed; NRA LOH & Patron Member, Golden Eagle, Patriot's Medal.
NRA Second Amendment Task Force Charter Founder
IHMSA and NRA Metallic Silhouette maker & member.
http://lufkinced.com/
anon45678@xxxxxxxxxxxxxx wrote:
ASSESSMENT COMMENTS ON METALLURGICAL ANALYSIS AURORA, TX ALUMINUM.
SAMPLE
Anonymous, PA, 2008
1.1 Introduction
In 1973, samples from a mass of aluminum were sent by John F.
Schluesser to several metallurgical labs for analysis. From the
photographs it appears to be an irregular chip-like mass approximately
3 cm x 2 cm by 1 cm. In the published documents, it is claimed to
have been received from Bill Case of Dallas, TX on June 19, 1973. Mr.
Case reportedly found it beneath 4 inches of soil in a field in Aurora
TX, lodged against a limestone rock face.
Figure 1. Photographs of aluminum sample obtained from B. Case, 1973.
Numbers on top scale correspond to 0.1 inch.
As this was an amateur investigation, there is no documentation of
proof that the sample came from this location. Furthermore, as its
provenance is associated with Mr. Schuessler and Mr. Case, both
associated with studies of paranormal phenomena and hoaxes, it is
highly questionable that this sample was found in the location
stated. There is no information regarding the age of the sample.
Nonetheless, the sample did exist in 1973, and was subjected to
seemingly valid metallurgical analysis. It is on these results that
we comment.
1.2 Analytical Results
Figure 2. Sketch of sample and its sectioning into multiple samples
for analysis (Schuessler documentation 1973)
The sample was apparently sectioned and sent to several analysis
labs. The results are tabulated below.
1.2.1 EDAX Analysis
Robert J. Danmeller, Marion Russo, (organization not given)
In the documentation, it states this organization was given sample #2,
but from their sketches, however, it appears they may have been sent
sample #1. Analysis was conducted using SEM imaging and EDAX
composition analysis.Runs 1-4 were taken from the face of a surface
exposed by the sectioning, and correspond to the interior of the
sample. EDAX specra indicates strong Al peak with 2 secondary peaks
labeled Fe. Run 5 was taken from an exterior surface region.
Material Peak Actual (keV) Run 1interior Run 2interior Run 3interior
Run 4interior Run 5surface Reported(keV)
Mg Ka1 1.254 -- -- -- -- --
Mg K-edge 1.303 -- -- -- -- --
Al Ka1 1.487 4000* 4000* 4000* 4000* 4000 1.45 (Al)
Al K-edge 1.560 -- -- -- -- --
Si Ka1 1.740 -- -- -- -- 304 1.70 (Si)
Si K-edge 1.840 -- -- -- -- --
S Ka1 2.308 -- -- -- -- --
Pb Ma1 2.346 -- -- -- -- 194 2.35 (Pb)
Bi Ma1 2.423 -- -- -- -- --
S K-edge 2.470 -- -- -- -- --
Cl Ka1 2.622 -- -- -- -- 122 2.65 (Cl)
K Ka1 3.314 -- -- -- -- 161 3.30 (K)
K K-edge 3.608 -- -- -- -- --
Ca Ka1 3.692 -- -- -- -- 168 3.70 (Ca)
Ti Ka1 4.511 -- -- -- -- 615 4.50 (Ti)
Ti K-edge 4.965 -- -- -- -- 137 4.95 (Ti)
Cr Ka1 5.415 -- -- -- -- --
Mn Ka1 5.899 -- -- -- -- --
Cr K-edge 5.989 -- -- -- -- --
Fe Ka1 6.404 100* 200* 1400* 100* 217 6.40 (Fe)
Mn K-edge 6.538 -- -- -- -- --
Fe K-edge 7.111 -- 30* 200* -- 66 7.05 (Fe)
Ni Ka1 7.478 -- -- -- -- --
Cu Ka1 8.048 -- -- -- -- --
Cu K-edge 8.980 -- -- -- -- --
Zn Ka1 8.639 -- -- -- -- --
Zn K-edge 9.661 -- -- -- -- --
Pb La1 10.55 -- -- -- -- 54 10.55 (Pb)
Bi La1 10.84 -- -- -- -- --
Table 1. Peak intensities from EDAX analysis on metallurgical sample
taken at 4 interior locations (Runs 1-4) and one location on the
exterior surface (Run 5). Data in rightmost column are peak
locations reported, along with the material they were indexed to. (*)
indicates estimate from EDAX screen shots
Energy dispersive X-ray (EDAX) is useful for identifying the presence
of elements in an alloy, but quantitative composition measurement
requires careful calibration to known standards. Nonetheless, there
is no observable Cu or Zn found anywhere in the sample. This suggests
the sample is a pure Al-Fe alloy, with some surface contamination.
1.2.2 MDRL Laboratory
Ronald A. Weiss, Sr. Group Engineer, McDonnell-Douglas Research
Laboratory
The analysis was conducted by J.E. Holliday using X-Ray fluorescence
and soft X-Ray spectroscopy. It is stated they were given sample #1
Material XRay fluorescence Soft X-Ray spectroscopy
Al 0.95 0.98
Fe 0.05 0.01-0.02
Table 2. Composition of metallurgical sample determined by x-ray
analysis
In this analysis, Holliday reports the presence of cavities often
associated with shrinking, and an overall microstructure consistent
with solidification processing. He identifies small crystals of Fe-Al
intermetallic compound. It is noted they are more numerous near the
outer surface than in the interior. The percentage of Fe is higher in
the XRF signal because it samples the enitre cut surface, while the
soft X-ray spectroscopy samples only a 1mm x 3mm spot on the cut
surface, initially located in the interior of the sample. The second
phase inclusions are described as needle-like, but their sizes are not
given.
1.2.3 Spectro-Chemical Research Laboratories
3300 West Lawrence Avenue, Chicago IL 60625, Bernard B. Hauser
This analysis by an independent lab appears to have been ordered by
Art Bethke, (Motorola?). It is not clear if this sample is from the
same where this sample was cut from. Bethke later reported the
composition most closely matched the 2011 alloy. The standard
composition range for this alloy is shown for comparison the Table
below.
Material Sample Alloy 2011
Al balance balance
Cu 5.68 5.0-6.0
Zn 0.02 0.30 max
Fe 0.38 0.7 max
Si 0.26 0.40 max
Mn 0.02 (<0.05)
Ni -- (<0.05)
Mg 0.01 (<0.05)
Ti trace (<0.05)
Pb -- 0.20-0.6
Bi -- 0.20-0.6
Table 3. Measured composition of metallurgical sample, with commercial
aluminum alloy 2011 shown for comparison.
These results indicate the presence a large amount of copper, along
with other components that suggest this is likely a commercial alloy,
in contrast to the other analyzed samples.
1.2.4 Antsas Technical Services - EDAX analysis
Antsas Technical Services,
Another analysis via EDAX was conducted in 1994, again showing 2 Fe
peaks in addition to the primary Al, and an absence of other
materials. It is unknown if this data is from the same material
analyzed in 1973. The analysis indicates the sample is 99.5% Al, with
0.5% Fe.
2. DISCUSSION
Aluminum alloys containing significant concentrations of Fe have been
prepared and stuided in the laboratory at least since 1916[1].
Precipitates of the AlFe3 intermetallic compound were identified in
these alloys as early as 1919[2]. By the mid 1970's there were
several hundred papers in the literature concerning Al-Fe as an alloy,
owing to its interest as in intermetallic forming system[3], high
temperature structural applications, and a creep-resistant high
temperature conductor[5]. Such alloys consist of an aluminum matrix
into which are dispersed iron aluminide particulates, that form a
creep resistant microstructure enabling it to maintain structural
integrity at elevated temperature[5]. The class of structural
intermetallics compounds that includes iron aluminides (Fe3Al, FeAl),
along with related systems nickel aluminides (Ni3Al, NiAl) and
titanium aluminides (Ti3Al, TiAl) posess many attractive properties
for high temperature structural applications. The aluminum rich
composition favors formation of protective Al2O3 in oxidizing
environments, low density, high melting points, and high temperature
strength[6], and it is predicted they are the most likely to replace
superalloys in future applications. A key challenge is overcoming the
brittleness of pure single phase intermetallics at low temperatures
and developing improved fabrication techniques.
Given the low solubility of Fe in Al and their widely different
melting temperatures, producing a bulk alloy of these materials is
difficult. An overall composition of Al0.95Fe0.05 can be prepared via
solidification from a high purity melt above 700C containing Al and Fe
in these quantities, or via powder metallurgy whereby Fe and Al
particles are milled together in a mechanical attrition process, then
sintered to form a bulk compact. In the metallurgical analysis of
1973, it is mentioned that the sample has large grains with needle-
like iron-rich strucutures. This is suggestive of a solidification
process where Fe-rich liquid segregates ahead of dendritic or cellular/
columnar solidification and forms extended iron-rich strucutres and
precipitates in the interdendritic/intercellular spaces. Powder
metallurgical microstructures typically would consist of a more
equiaxed microstructure with small Al grains interspersed with compact
AlFe or Al3Fe intermetallic particulates.
Figure 3. Fe-Al Phase diagram. Sample composition is on the aluminum-
rich end at Al0.95Fe0.05.
3. CONCLUSIONS
Technical
From the available metallurgical analysis documentation of 1973, it
appears
· The sample is an alumunum matrix composite with overall composition
Al0.95Fe0.05, with extended or needle-like Fe-rich structures, likely
an iron-aluminide intermetallic phase.
· Given the composition and microstructure this sample must have been
produced in a well-controlled metallurgical process, such as in a
laboratory.
· The capability to produce this material has existed since 1920, but
this composition would not have been widely available until sometime
after World War II. By 1973 it would have certainly been available to
someone with R&D connections in the aluminum or aerospace industries.
Relation to location of discovery
· The claim is that this metal sample was recovered from an 1897
'debris field' in Aurora TX, but there is absolutely no proof that
this sample is truly from this location. The sample discovery was not
properly documented and changed hands several times thus making it
useless for further study.
· Although Al-Fe alloys have been produced in research quantities
throughout most of the 20th century, they are not available
commercially, and therefore highly unlikely to have been deposited by
normal human activity in a rural area such as the location alleged.
· If the sample were truly collected from a debris field (for which
there is no proof) it is almost certain that additional amounts of
material would remain at the site. These fragments, likely in much
smaller sizes, perhaps 1 mm or less, would probably lie within the top
few cm of soil or embedded in rock faces. This alloy would also be
likely to remain relatively stable underground for decades.
· Although they may not be locatable by 'hobbyist' metal detectors it
is likely that archaeological excavation with fine particle fragment
collection techniques could discover additional samples of this alloy--
if it exists in a debris field of fine particulates.
· If new samples could be found (with proper on-site scientific
documentation), the crucial step would be to examine in detail the
composition and microstructure to ascertain with more certainty how it
might have been produced. Additional analysis to estimate the time
this material was in contact with the soil would be needed.
4. REFERENCES
1. O. Bauer and O. Vogel, "Aluminium-zinc alloys", Internationale
Zeitschrift fur Metallographie, v 8, n 3, p101-178, (1916).
2. P.D. Merica, R.G Waltenberg, J.R.Freeman, "Constitution and
metallography of aluminium and its light alloys with copper and
magnesium", Bulletin of the American Institute of Mining Engineers, n
151, p1031-1049, (1919).
3. S. Nasu, U.Gonser, P.H. Shingu, Y. Marakami, 57Fe Mossbauer spectra
in splat quenched Al-0.5, 1, 3 and 5 at% Fe alloys, Journal of Physics
F (Metal Physics), v 4, n 2, L24-28 (1974).
4. A. Olszowka-Myalska, J. Szala, J. Cwajna, Characterization of iron
aluminides formed in situ in an aluminium matrix compositMaterials
Characterization, v 56, n 4-5, p379-83 (2006).
5. R.W. Westerlund, "Effects of composition and fabrication practice
on resistance to annealing and creep of aluminium conductor alloys",
Metallurgical Transactions A (Physical Metallurgy and Materials
Science), v 5, n 3, (1974).
6. J.R. Davis, Heat Resistant Materials, ASM Handbook, 1997.
- References:
- Analysis of aluminum alloy sample Aurora TX
- From: anon45678
- Analysis of aluminum alloy sample Aurora TX
- Prev by Date: Analysis of aluminum alloy sample Aurora TX
- Next by Date: Re: Analysis of aluminum alloy sample Aurora TX
- Previous by thread: Analysis of aluminum alloy sample Aurora TX
- Next by thread: Re: Analysis of aluminum alloy sample Aurora TX
- Index(es):
Relevant Pages
|