Hi Randy:
I have come up against this same thing more than a few times doing stuff in
boats as well as dock ramps. You are using a Binzel push pull, so I wonder
if you are running it in front of a Powermig 300. If you are, what has
worked for me in the past is to set a long preflow so the joint is flooded
with argon and set your trim real low (almost ridiculously) so the wire
manages to get into the joint before arcing on the top and bottom. Also set
your arc control right to 10. Push your nozzle back as far as you can get
it ( contact tip protruding about 1/4" ). It takes a bit of practice but
once you get it, you may be surprised to see some of your best cosmetic
welds in what appears to be the most difficult place to put one.
(I am assuming that you are using .047 wire here) .035 doesn't seem to like
doing this for me for some reason.
If you are running conventional than just push tons of wire into it. Tons
of wire speed (ridiculous amounts for the voltage) to push the wire all the
way to the root of the joint.
Just out of curiosity, is this a truss for a ramp or bridge?
Drew McEachren
"R. Zimmerman" <m-zimmerman@xxxxxxx> wrote in message
news:yY1Bg.318305$iF6.182605@xxxxxxxxxxx
Has anyone made up an extension or modified gun nozzle and contact tip topull
reach into sharp corners. We have a four inch long seam to do that is
created by a four inch aluminum tube set at less then thirty degrees.
We tried out supplier but no smaller nozzles available. ( Binzel push
gun)stickout.
Presently the nozzle forces us to attempt a weld with a two inch
One can imagine the quality. Squeezing the tip of the nozzle will give usthreaded
about one and three quarters stickout... Still not enough.
I am toying with adapting a spool gun contact tip to the present
tip to five me a three inch long contact tip. The next step would be a
custom nozzle???
Randy
.
- Follow-Ups:
- Re: acute MIG joints
- From: R. Zimmerman
- Re: acute MIG joints
- References:
- acute MIG joints
- From: R. Zimmerman
- acute MIG joints
- Prev by Date: Re: What price for a used Millermatic 175 without tank?
- Next by Date: Re: making my own telescope type magnifiers?
- Previous by thread: Re: acute MIG joints
- Next by thread: Re: acute MIG joints
- Index(es):
Relevant Pages
|